A ZK60 magnesium alloy with an initial grain size of ≈10 µm is processed by high‐pressure torsion (HPT) through 5 revolutions under a constant compressive pressure of 2.0 GPa with a rotation speed of 1 rpm. An average grain size of ≈700 nm is achieved after HPT with a high fraction of high‐angle grain boundaries. Tensile experiments at room temperature show poor ductility. However, a combination of reasonable ductility and good strength is achieved with post‐HPT annealing by subjecting samples to high temperatures in the range of 473–548 K for 10 or 20 min. The grain size and texture changes are also examined by electron back scattered diffraction (EBSD) and the results compared to long‐term annealing for 2500 min at 450 K. The results of this study suggest that a post‐HPT annealing for a short period of time may be effective in achieving a reasonable combination of strength and ductility.