In this study, dynamic hydrogen bubble templating (DHBT) was deployed for thin film nickel electrodeposition on a nickel foil substrate. The DHBT of nickel electrodes was carried out on an opensource programmable rasterable system. Platinum wire (Ø = 0.1 cm) was used as the anode (counter-electrode), and nickel foil (6 x 6 cm and 0.0015 cm thickness) on graphite block was used as the cathode (working electrode). Symmetrical circles (Ø = 0.2 cm) in the order of four, three, two, and one were punctured on different polyethylene films, respectively. The polyethylene was used to mask the surface of the substrates, hence creating four different substrates. The corresponding current densities for the four different substrates are: 0.5 A/cm2 for the four symmetrical circles substrate, 0.7 A/cm2 for the three symmetrical circles substrate, 1 A/cm2 for the two symmetrical circles, and 2 A/cm2 for the one circle substrate. The nickel film electrodeposition time on each circle of the substrate was 250 secs, and the height of electrodeposition was 0.2 cm. Scanning electron microscopy was used to characterize the nickel film's topography and morphology, and an analytical balance was used to weigh the quantity of film deposition on the substrate. The result demonstrated that the amount of nickel deposited across the surface of the substrate varied based on the position of the counter-electrode. An uneven nickel film on the substrate occurs due to inequalities in hydrogen bubble generation, electrode placement, and localized concentration gradients. Profilometer imaging of the substrate showed the variability in discrete nickel deposits that characterize the non-linear deposition. While analytical methods were employed to characterize the substrate features and the film thickness, this study also presents a support vector regression and XGBoost machine learning to predict the thickness and percentage of nickel deposits on each substrate. Figure 1