Shallow arsenic junctions were formed in short processing times using gas‐phase rapid thermal diffusion with arsine or tertiarybutylarsine (TBA). A 60 s gas‐phase diffusion at 1100°C using 3.6% arsine in helium at 760 Torr formed 150 nm junctions with a measured sheet resistance of 100 Ω/□. Shallow junctions were also formed with a 12 min diffusion at 900°C using 10% TBA in argon at 10 Torr. These TBA‐formed junctions have arsenic concentration at the silicon surface greater than and a sheet resistance of 244 Ω/□. In addition, TEM cross sections show no process‐induced damage at the junction for gas‐phase doping.