Among the different components of a Solid Oxyde Electrolysis Cell (SOEC), the contact layer has a key role of insuring contact between the cells and interconnects. It thus should have a high electrical conductivity with minimum contact resistance. It can be achieved only if the material has a structural and chemical stability under the electrode working conditions, at temperature and under gas present in the chamber. Our study focuses on properties evolution of La 0.8 Sr 0.2 MnO 3 (LSM) material, which is one of the most used material for contact layer, under representative SOE system atmospheres. A thick layer of LSM was thermally pressed on a substrate of CroFer 22 APU to ensure good mechanical contact. The LSM layer was then annealed, following a thermal treatment similar to normal working condition of a SOFC, under a constant gas flow. Different type of gas flow were used to study its impact on the LSM structure. Several characterization methods on the annealed layers allowed evaluating the chemical and structural evolution after annealing. Our first analysis showed important changes in chemical and structural properties of LSM layer after annealing, depending on the oxygen partial pressure in the atmosphere. Under a gas flow of nitrogen or argon, the expected crystal phase (La 0.8 Sm 0.2 MnO 3 ) decreased in intensity, with the formation of other undesirable phases. When the quantity of oxygen is even further decreased, under a flow of Ar/H 2 , the crystal structure of LSM disappeared completely with only side phases detected. On the other hand, after annealing under a constant flow of compressed air, the LSM phase is as pure as after its synthesis, without any other phases detected. Cycles of thermal treatment under different gas flow showed a reversibility of phases, with however a detrimental impact on the adherence of the film on the substrate. This can be due to the variation of phases with different crystal sizes and different thermal dilatation. It induces constraints in the film that leads to its delamination from the substrate. This phenomenon indicates that a variation of the working atmosphere of an SOEC, ie. from its preparation to the production of H 2 , can have a major impact on the mechanical stability of the contact layer, which directly impacts the performances of the SOFC. Introduction Hydrogen could play a pivotal role as a supply to reduce carbon footprint of many industrial processes, among other applications such as transportation fuel and long-distance and large energy storage [1]. However, 95% of current production of H 2 is produced from fossil fuels, emitting a lot of CO 2 . Production of carbon-free hydrogen needs to be further developed to increase its deployment in new domains. High temperature water electrolysis may be the prime way for large and cost-efficient clean production of H 2 . To be competitive with carbon-based methods, production costs should be reduced as much as possible. SOEC is a good candidate in this regard, as the exploitation of free heat and water vapor helps to reduce the cost and the energy to bring for water splitting, and thus the amount of electricity needed for the electrolysis [2]. Among the different materials studied for cathode and/or contact layer for SOEC, perovskite-type oxide, La 1−x Sr x MnO 3 (LSM), is a prime candidate due to its high electronic conductivity, chemical compatibility with zirconia-based electrolytes and catalytic activity for oxygen reduction [Ref]. Despite its importance for SOEC, there is limited literature about the microstructure of LSM and the impact of oxygen partial pressure on it [3]. Most of works concern the powder preparation and stoichiometry [4, 5], the electronic conductivity [6] or crystal structure evolution using modelling [7, 8]. Here, we propose to determine the impact of oxygen partial pressure on the crystal structure of LSM experimentally and with material characterization methods. Experimental Lanthanum Strontium Manganite films A slurry of LSM were prepared from commercial powder of LSM acquired from Marion Technologies. The powder was dissolved in a solvent and milled. The formed slurry was then used for tape casting using a doctor blade. The height of the blade was fixed to obtain a film’s thickness of 250 µm. Films were laser cut in square of 30 cm² to fit the size of CroFer 22 APU substrate. The mechanical contact between films and substrate was assured by thermal pressure. Annealing Samples were annealed in a homemade cubic oven, tightly sealed from outside atmosphere, with a programmed heating cycle corresponding to a 1°C/min ramp up to 850°C, a 1-hour plateau, a decrease to 800°C, a second 1-hour plateau and a decrease to room temperature. Cycles were performed under a constant gas flow, of either N 2 , Ar, 97%Ar/3%H 2 or compressed air. Inert atmosphere is often used in both chamber of a SOEC before applying working condition, with an evolution of the O 2 compartment to a more oxygen-rich atmosphere. Moreover, a reducing atmosphere may appear with inter atmosphere in O 2 chamber and a leak between chambers. The atmosphere in the chamber was controlled with a pressure sensor to ensure that the chamber is at higher pressure than outside room, to make sure that no air from the room entered the oven. Characterization Crystal structure of LSM films were recorded with an Empyrean XRD from Malvern Panalytical, with Cu kα x-ray generator and a PIXcel detector in gonio scan from 20 to 120° theta. XRD peaks association was made using Highscore Plus software and the PDF database. Results 2.1 Annealing with 1 thermal cycle Thermally pressed LSM films on CroFer 22 APU undergo a thermal treatment cycle with a 1-hour step at 850°C followed by another 1-hour step at 850°C under different gas flow (N 2 , Ar, 97%Ar/3%H 2 and compressed air). Afterward, the crystal structure was measured by XRD, the resulting spectra are displayed in Fig.1, with the addition of a spectrum before annealing, as a reference. The XRD spectra of the film before annealing corresponds to a pure LSM (PDF file 00-074-1204), with high crystallinity as seen from the intensity of peaks, without any other peaks. After an annealing under a constant flow of air, a corresponding XRD spectrum was measured, indicating a stability of LSM in oxygen-rich atmosphere, as it would undergo in SOEC working condition. In a low PO 2 atmosphere, under either N 2 or Ar flow, both displaying similar XRD spectra, the crystal structure of the film is modified, with a decrease in intensity and modification of LSM peaks and the formation of new peaks, which do not fit the LSM crystal structure reference. This could indicate a degradation of LSM crystal structure and its modification in other phases. When annealing a LSM film in Ar/H 2 , which is a very low PO 2 atmosphere, no XRD peaks can be attributed to LSM, indicating a complete degradation of the original crystal structure. The LSM crystal structure appears to be very sensible to the quantity of oxygen present in the atmosphere, with a stability only in oxygen-rich environment, and its degradation following the decrease of oxygen concentration. These 2 annealing didn’t have any impact on the physical stability of LSM films on the CroFer support. 2.2 Annealing with 2 consecutive cycles To simulate a change in atmosphere, a second thermal cycle with compressed air flow has been realised on a LSM film primarily exposed to a first thermal cycle under constant N 2 flow. and. The resulting XRD spectra is displayed in Fig. 2a. The crystal structure corresponds to a pure LSM phase, without any XRD peaks that do not fit the reference (Fig.2a). This indicates a reversible structure of the film when annealing in atmospheres with variable oxygen concentration. Although the analysed crystal structure corresponds to LSM, when taking the sample out of the oven, the LSM films was completely detached from the substrate (Fig.2b). Delamination occurred during the second annealing cycle. The rupture of the LSM layer happened at the interface with the CroFer substrate, as controlled by Scanning Electron Microscope (picture not shown), with some particles of LSM still left on the surface, inducing a darker color of the CroFer surface. No modifications of adherence occurred when annealing LSM films with 2 thermal cycles under a constant atmosphere (either Ar or air). Discussion These first experiments on the thermal behaviour of the LSM layer indicate important evolution of its microstructure, leading to its instability and complete loss of contact of most of the film with the support. It can have an important impact on the way stacks are handled, before and after working conditions. Several factors can explain this behaviour. Crystal structure measurements seems to show that the LSM is stable only in oxygen-rich environment, with important degradation following the decrease of oxygen concentration in the atmosphere. Under a flow containing very low amount of oxygen, at high temperature, the LSM structure appears to be heavily modified, as shown in XRD measurements. Firstly, the LSM structure is impacted under inert atmosphere at high temperature. The most important change is the creation of oxygen vacancies in the crystal structure under a dry atmosphere. [6] When the oxygen partial pressure decreases, the reaction (1) of reduction is pushed to the right, with the increase of oxygen vacancies ([V ••O ]) and the Mn 3+ (Mn ×B ) valence on the B site of the perovskite, while the Mn 4+ (Mn •Mn ) valence and the O 2− ion on the oxygen site (O ×O ) will decrease: (1) 2 Mn •Mn + O ×O = 2 Mn ×B + [V ••O ] + 1/2 O 2 The oxygen vacancy was reported to be ~ 30 ppm in air and ~ 2000 ppm in Ar at 1100°C. [8]. The formation of oxygen vacancies and the change of charge for Mn have a major impact on the volume of the cell. LSM weight loss during thermal cycles between 800°C and 1100°C in Ar was measured of 0.272%, and only 0.083% in air, mostly from oxygen vacancies, whereas the ionic radius of Mn 3+ was reported to be more than 10 pm higher than those of Mn 4+ [8]. Secondly, XRD measurements has indicated the formation of other phases within the film after annealing in low oxygen atmospheres. According to the equilibrium phase calculated by Grundy et al [7], these phases could correspond to La 2 O 3 , SrO and MnO, but also phases with stoichiometry modification of LSM, such as (La, Sr) 3 Mn 2 O 7 . These phases probably have crystal volumes different from LSM. When cycling from oxygen-rich to an oxygen-poor atmosphere, these changes in crystal volume must induces strong constraints in the LSM film that are released in the complete delamination of the film from the substrate. Delamination that could have a detrimental impact for the electrical conductivity. Thus, considerations should be taken into account when manipulating SOEC stacks before and after working conditions. Further experiments are ongoing to be closer to SOEC working conditions, ie. a LSM annealing with cycling N 2 and air under an applied pressure and with LSM surface engineering, such as channels to leave space on sides for the crystal volume variation. References [1] J. Mougin, Chapter 8 in Compendium of Hydrogen Energy, Volume 1: Hydrogen production and purification, Elsevier, 2015 [2] A. Odukoya, et. al., Int. Journal of hydrogen energy 41 (2016) 7878-78 [3] T. Grande, et al., Chemistry of Materials 24, nᵒ 2 (2012): 338-45. [4] Mizusaki, et al., Solid State Ionics 129, nᵒ 1 (2000): 163-77. [5] McCarthy, et al., Journal of the American Ceramic Society 92, nᵒ 8 (2009): 1672-78. [6] Darvish, et al., Journal of The Electrochemical Society 162, nᵒ 9 (2015): E134. [7] Grundy, et al., Calphad 28, nᵒ 2 (2004): 191-201. [8] Zhong, et al., JOM 74, nᵒ 12 (2022): 4533-43. Figure 1