Sulfidation Behavior of Fe-25Cr-20Ni-3Si in H2/H2O/H2S/Ar at 700°C

Authors:

Abstract
The isothermal and cyclic sulfidation behavior of Fe-25Cr-20Ni-3Si and Fe-25Cr-20Ni (wt%) was studied at 700°C in several H2/H2O/H2S/Ar gas mixtures. A range of partial pressures of oxygen, 1.17 x 10–20 to 1.18 x 10–22 atm was used at a constant sulfur potential of 1.22 x 10–8 atm. Alloy coupons with and without preoxidation were exposed to the gas mixtures for times up to 192 h. Alloys were preoxidated for up to 96 h at 700°C in an H2/H2O/Ar gas mixture with pO2 = 1.13 x 10–20 atm. The oxide scale and corrosion products were analyzed using SEM/EDAX, XRD, SAM, and SIMS. A remarkable sulfidation resistance in the case of Si-containing alloy was observed under the conditions examined, and the interpretation of this observation is discussed. The base alloy, Fe-25Cr-20Ni, underwent sulfidation within a few minutes of exposure to the bioxidant gas mixture, beginning at the gas/scale interface.