Pressureless Sintering and Reaction Mechanisms of Ti 3 SiC 2 Ceramics

Authors:

Abstract
Easy sinterable Ti 3 SiC 2 powder was synthesized from a powder mixture with a molar ratio of 1.0 Ti , 0.3 Al , 1.2 Si , and 2.0 TiC by heating at 1200°C in the flowing Ar. Here, the Al powder acts as a deoxidation agent and provides a liquid phase for the reaction. The powder compacts subjected to pressureless sintering at 1300°C in Ar had a relative density up to 99%. The results of chemical analysis and the measured lattice constant suggest that the Al–Si liquid phase was formed at approximately 1200°C and that liquid‐phase sintering was promoted by the 0.1 molar ratio of Al and the 0.2 molar ratio of Si remaining in excess. The three‐point bending strength, fracture toughness, and electrical resistivity of the sintered samples were 380 MP a, 4.1 MP a m 1/2 , and 0.34μΩm, respectively.
Funding Information
  • Japan Society for the Promotion of Science (23350104)

This publication has 32 references indexed in Scilit: