The following conclusions are obtained: 1. The autohesion strength of elastomers increases linearly with the rate of detachment over the range 200 to 1000 mm/s. 2. The autohesion strength increases by a factor of only 2× to 3× when the contact pressure is increased by 3 orders of magnitude, from 2 kPa to 2 MPa. 3. Autohesion strength develops rapidly in the early stages of contact for SBR, BR, and EPR, increasing from about 20 J/m2 to about 500–1000 J/m2 as the contact time increased from 1 to 100 ms. It increased more slowly thereafter, to about 10 kJ/m2 after a contact time of 1000 s. 4. The development of autohesion was exactly the same at 3°C as at 25°C. This feature is attributed to simultaneous changes in developing true contact, and in resisting separation after contact, that exactly cancel. 5. Adhesion between SBR and EPR is lower than the autohesion strength of the individual polymers over the whole range of contact time. On the other hand, the three strengths for SBR and BR are almost the same. 6. The overall similarity between the rates of development of autohesion and adhesion suggest that autohesion is governed mainly by the strength and extent of intimate molecular contact that is developed at the interface. Contributions from interdiffusion, if any, appear to be significant only in the later stages of contact.