Thin oxide layers have been grown on atom probe needles of Zircaloy in order to study the oxide-metal interface. The oxide was formed during one to thirty days in dry air, as well as during 5 s in boiling water. Atom probe analysis was performed of oxide layers thinner than 10 nm. These layers were found to contain low amounts of oxygen, less than stoichiometric ZrO. Transmission electron microscopy of equally treated specimens showed that the oxide was partially amorphous and contained small crystallites 5-10 nm in size