SiC thick films of about 300 μm could be prepared with a deposition rate above 300 nm/s by thermal plasma physical vapor deposition (TPPVD) using ultrafine SiC powder as a starting material. The thermoelectric properties were investigated as a function of composition and doping content. The nondoped films showed n-type conduction. Although the Seebeck coefficient reached as high as −480 μV/K, the power factor was only around 1.6×10 −4 W m −1 K −2 at 973 K due to the relatively high electrical resistivity. In order to reduce the electrical resistivity and to deposit layers with n-type and p-type conduction, N 2 , B and B 4 C were selected as the dopants. Nitrogen-doped samples exhibit n-type characterization, B and B 4 C-doped samples exhibit p-type characterization, and the electrical resistivity decreased from 10 −2 –10 −3 to 10 −4 –10 −5 Ω m after doping. The maximum power factor of the nitrogen-doped SiC and the thick films deposited with B 4 C powder reached 1.0×10 −3 and 6.4×10 −4 W m −1 K −2 at 973 K, respectively. Keywords Thermal plasma physical vapor deposition Silicon carbide Thermoelectric properties 1 Introduction There is a growing interest in thermoelectric power generation, which allows direct conversion of thermal energy into electrical energy. Thermoelectric energy conversion has many technical advantages over other methods. For example, the devices can generate electric energy without any exhaust gases and do not contain any movable parts; therefore, no mechanical vibration and no noise are produced. Also, they are reliable for long periods without requiring maintenance. Materials such as Bi 2 Te 3 , SiGe and FeSi 2 have reached the practical application stage. However, the materials developed so far are easily oxidized, decomposed or melt above 1000 °C and thus limit the efficiency of the devices. Increasing the temperature difference can improve the efficiency. Therefore, the development of high temperature thermoelectric materials is of special interest. Recent development and investigations showed that SiC and B 4 C are promising candidates for high temperature applications because of their high thermoelectric power, high thermal stability, high resistance to oxidation and corrosion, and their nontoxicity [1–7] . So far, the main work on SiC as a thermoelectric material is focused on sintered SiC. However, SiC is relatively difficult to be sintered. We have successfully deposited nanostructured and thick SiC films by a novel process—thermal plasma physical vapor deposition (TPPVD), with SiC ultrafine powder as a starting material [8,9] . In this study, we report the results of thermoelectric properties of these thick SiC films. 2 Experimental procedure The SiC thick films were deposited in a hybrid plasma processing system which has been previously described in detail [8,10–11] . Ar (55 slm) and hydrogen (4 slm) gas mixture was used as the plasma gas. Using Ar as the carrier gas, silicon carbide ultrafine powder with the average particle size of around 0.1 μm (Sumitomo Osaka Cement Co. Ltd) was fed into the plasma jet, completely evaporated and transported to the graphite substrate surface located 35–75 mm from the plasma torch exit. The powder feeding rate varied from 10 to 120 mg/min. In order to control the C/Si atomic ratio of the SiC films, methane with a flow rate in the range from 0 to 500 sccm was injected as the plasma gas. The chamber pressure was maintained at a constant pressure of 250 Torr. The substrates were preheated several minutes by the plasma flame before deposition. The temperature was measured with a pyrometer. In order to prepare films with n-type and p-type conduction and to improve the thermoelectric properties, nitrogen, B and B 4 C were used as the dopants. Nitrogen flow rate was in the range between 0 and 500 sccm. The purities of both B and B 4 C were 99%, and the average particle sizes were around 1 and 10 μm, respectively. The deposited films were examined by scanning electron microscopy (SEM), X-ray diffraction (XRD) and X-ray photoelectron spectroscopy. The samples for thermoelectric measurements were mechanically ground with emery paper and diamond polisher to get rid of the graphite substrate completely, and then mounted on a ceramics holder using Pt paste. The thermoelectric power, S , and the electrical resistivity, ρ , were measured in helium atmosphere using the thermoelectric power measurement apparatus ZEM-1 (ULVAC). The measurements were performed with the samples heated from room temperature to 973 K and then cooled to room temperature in steps of 50 or 100 K. Temperature differences of 20 and 40 K were applied to the two ends of the sample holder to measure the Seebeck coefficient for each temperature point. The power factor was calculated from the Seebeck coefficient and electrical resistivity. 3 Results and discussion 3.1 Preparation and structure characterization of SiC films Fig. 1 shows the SEM fracture morphology of typical samples of nondoped, nitrogen-doped, B-doped and B 4 C-doped SiC films deposited at RF power of 70 kW. The nondoped samples exhibit columnar structure, as shown in Fig. 1(a) . Nitrogen doping had little influence on the cross-sectional morphology (see Fig. 1(b) ). The B and B 4 C additives significantly improved the dense cross-sectional morphology, as shown in Fig. 1(c) and (d) , even though a layer-by-layer structure was developed for B 4 C-doped films. Fig. 2 shows the influence of the N 2 flow rate on the deposition rate with various amounts of methane injection. It can be seen that as nitrogen content in the plasma increased, the deposition rate decreased dramatically. This is due to the escape of the C source in the gaseous form of CN. The maximum thickness of the B 4 C-doped dense layer reached 320 μm and a deposition rate of around...