Hysteresis loops in fields to 100 kOe have been measured at 300, 77, and 4.2K parallel and perpendicular to the alignment axis in a series of sinteered SmCo5 magnetis with compositions varying from 16.24 to 17.08 at% Sm. Analysis of the data taken perpendicular to the alignment axis permits evaluation of the effective anisotropy constant K1, and also the degree of misorientation of the individual particles. Intrinsic coercive fields Hci varied from 0.34 to 16.4 kOe at room temperature. In all samples, Hci and K1 increased rapidly with decreasing temperature, roughly doubling between room temperature and 77K. This confirms more generally the result reported for two samples by Benz and Martin.1 The values of Hci and (BH)max depend strongly on composition, but the anisotropy does not. Variations in permanent magnet properties are therefore not directly related to variations in the bulk anisotropy.