Abstract
In this work, we report on the ablation of a tungsten target with a nanosecond Nd:YAG laser of high intensity, ranging from 2 × 10 8 to 10 11 W/cm 2 , at 355 nm wavelength. We use a microbalance device and SEM to analyze the phase explosion mechanism. The microbalance was placed in front of the target where the maximum ejection of matter took place. The results obtained showed two kinds of ablation process: normal surface evaporation at low laser intensity (below 10 10 W/cm 2 ) followed by explosive boiling (also called phase explosion) at a threshold laser intensity of 6 × 10 10 W/cm 2 . The analysis of the surface crater formed by 1, 5 and 10 laser shots on the target at high laser intensity by SEM showed that the morphology of the crater consists of pores and cavities which are due to bubble nucleation when the critical temperature of tungsten is reached. These bubbles are the characteristic of phase explosion transformation. Copyright © 2010 John Wiley & Sons, Ltd.