Abstract
Eleven U.K. laboratories performed dry pin-on-disk wear tests on a 95% alumina ceramic under a load of 40 N and at a sliding speed of 0.1 ms-1. Specimens were supplied with polished and ground finishes; the ground finish gave higher wear and lower friction than the polished specimens. Subsidiary experiments showed a large effect of humidity on wear with high wear rates at low humidity levels. The measure of wear with the best repeatability was scar size measurements at 5%, and the worst was mass loss measurements at 42% (expressed as ratios of 95% confidence intervals to the mean values). The reproducibility of friction measurements was 14%.