Metalorganic Chemical Vapor Deposition of BaTiO3 Films on MgO(100)

Authors:
  • HNHidenobu Nakazawa
    Hidenobu Nakazawa
  • HYHisanori Yamane
    Hisanori Yamane
  • THToshio Hirai
    Toshio Hirai

Abstract
BaTiO3 thin films were prepared on MgO(100) substrates by chemical vapor deposition using barium β-diketonate {Ba(C11H19O2)2} and titanium tetraisopropoxide {Ti[OCH(CH3)2]4} as metalorganic precursors. BaTiO3 films deposited at 800-1000°C showed prominent a-axis orientation perpendicular to the substrate surface. The deposition rate of these films was 1.0-1.2 µm/h. The rocking curve of BaTiO3(200) reflection from the film deposited at 800°C indicated strong crystallographic orientation. The epitaxial relationship between the film and the substrate was found by X-ray pole figure analysis. The relative dielectric constant of a polycrystalline BaTiO3 film prepared on a Pt(100)/MgO(100) substrate at 800°C was 1040 (10 kHz, 20 V/cm).

This publication has 14 references indexed in Scilit: