Lattice parameter changes in the mixed-oxide system Ce1–xLaxO2–x/2: a combined experimental and theoretical study

Authors:
  • BMBelinda C. Morris
    Belinda C. Morris
  • WFWendy R. Flavell
    Wendy R. Flavell
  • WMWilliam C. Mackrodt
    William C. Mackrodt
  • MMMichael A. Morris
    Michael A. Morris

Abstract
X-Ray diffraction measurements are reported of ceramic samples of the mixed-oxide system Ce1–xLaxO2–x/2 for 0<xx has been determined by EDXA. The solid-state reaction forms a highly crystalline product at an ageing temperature of 1200 °C. The solubility limit of La in the bulk CeO2 at this temperature has been determined as ca. 52% by monitoring the lattice parameter increase and the subsequent appearance of a second La2O3 phase. To model the experimental measurements, atomistic lattice calculations based on electron-gas shell-model potentials have been carried out to estimate the variation of the lattice parameter with La content.

This publication has 14 references indexed in Scilit: