The corrosive conditions to which chemical evaporator tubes may be exposed on the steam side were simulated in corrosion tests run in hot water saturated with mixtures of carbon dioxide and air under pressure. These showed that appreciable corrosion of nickel can occur in a critical range of composition of the non‐condensable gases, namely from about 55 to 90 per cent carbon dioxide by volume. In the presence of iron corrosion products, this range is broadened to include 40 to about 90 per cent carbon dioxide. Outside the critical range, nickel owes its good resistance to development of a passive film. Corrosion of nickel can be prevented by removing air or carbon dioxide from steam until their ratio is no longer critical. Inconel, tin, and stainless steel were resistant to attack under all the experimental conditions. Zinc and some copper alloys were also tested.