Localized discoloration of LEDs in an LED-TV backlight unit was investigated as a field failure. FE-SEM/EDX showed silver and sulfur co-located in the discolored region, and cross-sectional TEM/EDX showed the reaction product extending from the Ag-plated lead-frame into the phosphor layer, consistent with Ag2S. Purge-and-trap GC–MS of the reflective sheet and the LED mounting board, measured together under reflow-representative conditions, identified 9H-thioxanthen-9-one, released intact, as the only sulfur-bearing volatile; no sulfur species was found in the package materials. Pyrolysis GC–MS of the sheet alone at 500–600 °C detected no sulfur-bearing compound, which assigns the carrier to the board's UV-cured solder resist, a coating in which thioxanthones serve as photoinitiators. Cross-sections of the failed packages showed interfacial delamination between the silicone lens, the reflective cup and the lead-frame, and dye penetration at ambient pressure, which fills only an end-to-end open path, confirmed that this pathway is continuous to the internal cavity in failed units and closed in the normal comparison unit. A transport analysis separates the two candidate routes by time lag alone: 0.07 s along the 2.6 mm seam against 170–1700 s through the 1 mm of intact silicone, itself several times the 63 s the package spends above 220 °C. That comparison is independent of how strongly the carrier partitions into the encapsulant, so it is the delaminated interface rather than encapsulant permeability that governs whether sulfur reaches the metal. A temperature-weighted mass balance on the measured 4.75 µm gap shows that one 260 °C reflow excursion delivers enough sulfur for ≈190 nm of Ag2S at full conversion, so the observed film requires a C–S scission yield of some tens of per cent, with scission surface-mediated at undercoordinated silver sites rather than on close-packed terraces. Sulfur outgassing from the mounting board and package interfacial integrity are coupled root causes.