Considering the difficulty of sintering and leachability of alumina―based ceramic core, different contents of silica were added to the specimens. The porous alumina―based ceramic core was prepared using the dry pressing processes. The effect of different contents of silica, sintering temperature and sintering time on the properties of the alumina―based ceramic core were investigated. The results indicated that the linear shrinkages of the specimens sintered at 1500¡䟡nd 1600¡䟦or 2 h were nearly the same. When the sample was sintered at 1700¡䟦or 2 h, the bending strength was decreased and the porosity was increased due to the evaporation of SiO2. The shrinkage, bending strength, porosity and bulk―density of the specimens sintered at 1500¡䟷ere invariable when the holding time exceeded 4 h. The sample sintered at 1500¡䟦or 2 h had linear shrinkage of 1.1%, bending strength of 63 MPa, the porosity of 35.5% and bulk―density of 2.29 g/cm3, which was hopeful to be the core candidate materials in high temperature application