The study investigates the high‑temperature interaction between liquid Al and Al-7Si alloy and a compacted Ti+C substrate using the sessile drop method with non‑contact heating and capillary purification at 800 °C under high vacuum. Both Al/Ti+C and Al-7Si/Ti+C systems initially exhibited non-wetting behavior (40 s and 150 s, respectively), followed by reactive wetting, with contact angles decreasing to 40° for Al and 60° for Al-7Si. The transition is governed by reaction-controlled spreading at the drop/substrate interface. SEM and TEM analyses revealed that interfacial reactions are dominated by Al-Ti and Al-Ti-Si phase formation. TiAl3 formed in the Al/Ti+C couple, while the Al-7Si/Ti+C system produced Si-enriched α-Ti and Ti(Al,Si)3, explaining the ~550 s delay in spreading. Localized TiC formation occurred due to transient thermal fluctuations enabling short-range Ti-C diffusion. Additionally, oxide films were shown to significantly influence high‑temperature wettability behavior.